By Robin WenReviewed
Tungsten Carbide Production: Carbon Budget
Carbon is set when tungsten is carburised, lost when the powder is milled, and only visible in the finished part when a brittle eta phase appears.

On this page
Tungsten carbide production is usually described as a sequence of temperatures: reduce, carburise, mill, sinter. That description is accurate and incomplete, because the quantity that decides whether a finished insert is tough or brittle is not a temperature. It is carbon, and it is set, lost and restored at three separate points along the route that makes tungsten carbide powder into a tool.
The arithmetic of the compound shows how thin the margin is. Tungsten carbide is 6.13% carbon by mass — 12.011 divided by 195.85 — and a typical WC-9Co grade with 1% chromium carbide reports 5.517% total carbon in the sintered part (Stanciu et al. 2025). Since the tungsten carbide fraction is 90% of that grade, 5.517 ÷ 0.90 gives 6.13. The carbon is not approximately right; it is stoichiometric, and a working tolerance of a tenth of a percent is therefore about 1.6% of the carbon that is supposed to be present.
Tungsten carbide production starts at 1300 °C, and the powder comes out agglomerated
The conventional route begins with tungsten metal powder, produced by calcination and hydrogen reduction of the oxide, and carburises that metal at 1300–1400 °C under hydrogen. The Stanciu review gives the size relationship directly: the size of the obtained powder depends on the size of the tungsten particles subjected to carburizing
. Grain size in the finished tungsten carbide insert therefore begins as a decision about the metal powder, two process steps upstream of the part.
The tungsten carbide leaving the furnace is somewhat agglomerated
and requires grinding to reach the desired particle size distribution
. This is where tungsten carbide production stops being a heat treatment and becomes a mechanical process. Milling is also where carbon first becomes exposed, because fresh surface is created in an atmosphere that contains oxygen.
Milling removes carbon indirectly, by putting oxygen in
The mechanism is stated plainly in the review’s own failure analysis of its reactive-sintering samples, where the review calls eta phase an undesirable, fragile carbide of the M6C or M12C type
and is traced to oxygen absorption on the surface during milling, which is reduced by carbon from the carbides
. Carbon is consumed reducing oxide that formed on particles that had just been fractured. The carbon that did this job is no longer available to form tungsten carbide.
The consequence has a name and a formula. Eta phase is a carbon-deficient carbide of the M₆C or M₁₂C type, where the metal-to-carbon ratio has drifted below one, and it is brittle. The Stanciu samples milled with steel balls carried more of it than samples milled with heavier WC-Co media — measured as up to 2 wt.% of W₆Co₆C in the steel-milled tungsten carbide — even though both were milled for the same ten hours.
Two fixes exist and they cost different things. The first is to add carbon back: the addition of 1.5-2 wt.% of graphite eliminated the η-phase and improved densification and hardness
, per the Trung work cited in the Cahill study on eta-phase suppression, though that work were only able to obtain relative densities up to 94.5%
. The second is to control the sintering atmosphere’s carbon potential, which is why furnaces for tungsten carbide are specified with gas control rather than as plain vacuum vessels.
Sintering consolidates what milling has already decided
Sintering runs near 1450 °C, hot enough for the cobalt to melt, and the review describes what happens when carbon runs short at that temperature: the absence of carbon results in a higher dissolution of tungsten into cobalt, the appearance of more liquid phases, and an increased eta phase during solidification
. The chain matters more than any single step. A shortage created by milling oxygen shows up as a phase that forms while the tungsten carbide part cools, in a furnace, hours later.
This is why the powder specification cannot carry the whole answer. A certificate can state a carbon percentage and a particle size, and neither reports how much oxygen the tungsten carbide picked up in the mill or how much carbon that oxygen consumed. The chemistry that governs the part is a process quantity spread across three machines.
| Stage | Temperature | What happens to carbon | When it goes wrong |
|---|---|---|---|
| Carburising | 1300–1400 °C, hydrogen | Fixed at stoichiometry; powder agglomerates | Coarse tungsten gives coarse tungsten carbide |
| Milling | Ambient, in solvent | Consumed reducing surface oxide | Local shortage, seeds eta phase |
| Sintering | ~1450 °C, vacuum then Ar/H₂ | Redistributed in the liquid binder | Eta phase on solidification; embrittlement |
Grain size is held by an inhibitor, which is a solubility argument
Cobalt content and grain size are the two axes a tungsten carbide grade is bought on, and the second is not controlled by milling harder. Chromium carbide added to the cobalt limits the solubility of tungsten carbide during sintering, acting as a grain growth inhibitor
. Vanadium carbide and tantalum carbide work on the same principle. A grain grows because tungsten carbide dissolves into the liquid cobalt and reprecipitates onto larger grains; slow the dissolution and the growth slows with it.
The measured difference between two milling media in the same study is a factor of about two in grain size — 0.70 µm for steel balls against 0.32 µm for WC-6Co balls — and the explanation given is energy: WC-Co balls are twice as heavy as steel balls
, so more of the mill’s energy reaches the powder. Hardness followed at 1,762 against 1,809 HV30, with toughness at 10.9 MPa·m1/2. Typical values for this composition family run from 1,000 to 1,900 HV.
The short cut merges two steps and pays for it in density
Reactive sintering skips the carburising furnace. Tungsten, carbon and cobalt are milled together for ten hours, pressed, and heated once, so that carbide formation and consolidation happen in the same cycle at 1450 °C for one hour under 95% argon and 5% hydrogen. Tungsten peaks are gone from the sintered diffractogram, which is the evidence that carburisation completed inside the sintering furnace.
The two routes differ in how many furnaces they use, and in what each one is asked to guarantee:
| Conventional | Reactive sintering | |
|---|---|---|
| Furnace passes | Carburising, then sintering | One |
| Atmosphere | Hydrogen for carburising | 95% Ar / 5% H₂ throughout |
| Carbon fixed by | Powder specification before pressing | The mix, with no second chance |
| Density reached | Above 99% with pressure assistance | 90% in the study, 70% with steel media |
What reactive sintering does not do is reach the density the industry requires. The samples consolidated with WC-Co media reached nearly 90%
against about 70% for steel media, and the review states the industrial requirement as +99%
. Pressure-assisted sintering closes that gap, at which point the saving of one furnace has to be weighed against a hot isostatic press.
Tungsten carbide is bought for wear, and the routes differ by buyer
The end uses do not all need the same tungsten carbide. USGS puts an estimated 60% of United States tungsten consumption into cemented carbide parts for cutting and wear applications, and the remaining share goes to mill products, alloys and chemicals. Within the cutting side, a coated insert for steel and an uncoated button for a drill bit are different products from the same powder: the first is a substrate for a CVD or PVD coating, the second is a wear part with a hardness gradient.
The named industries are the ones with a maintenance budget rather than a materials budget. Mining and construction consume the drill and wear parts; automotive consumes cutting tools for machining castings and gears; aerospace consumes both, plus tungsten carbide for components that need to survive abrasion at temperature. An abrasive grade — crushed tungsten carbide grit — is sold by size distribution rather than by cobalt content, and it shares the first two process steps with the tool grades and nothing after that.
Supply is concentrated, and the price moved in 2025
China remained the world’s leading producer of tungsten concentrates at 67,000 tonnes of tungsten content in 2025, against reserves of 2.5 million tonnes, and the United States depends on imports for more than half of apparent consumption, according to USGS. Import sources over 2021–24 were led by China at 26%, then Germany at 14% and Bolivia at 8% — Germany’s share being tungsten carbide and mill products rather than ore.
Prices moved sharply during 2025. The Rotterdam in-warehouse price for 65% WO₃ concentrate rose from $266 to $551 per metric ton unit, and USGS records $380 as the annual average for 2025 against $252 in 2024. China implemented new export controls on selected tungsten items in February 2025. For a tungsten carbide buyer the transmission is indirect — the concentrate price reaches the powder, not the insert — but it sets the floor under every quote in the chain.
Tungsten carbide production leaves three quantities to be checked
The vocabulary a supplier uses is narrower than the process, so three terms carry most of the risk:
- Total carbon — a single percentage for the whole part, checked against the stoichiometric value for the tungsten carbide fraction.
- Eta phase — a carbon-deficient carbide that appears when total carbon falls short locally, invisible to a chemistry certificate.
- Porosity class — an ISO letter and number for residual pore size, distinct from the density percentage quoted alongside it.
Three properties follow, and only the first is on the certificate:
- Cobalt content and grain size. These set the hardness-toughness trade and both are declared. Grain size in the finished tungsten carbide part is inherited from the tungsten powder, so it is fixed before the powder supplier ships.
- Carbon balance. Declared as a total carbon percentage against a stoichiometric expectation. A part can pass a certificate and still contain eta phase, because that phase forms during cooling from a shortage that happened upstream in milling.
- Density and porosity class. The review treats 90% as a laboratory result and 99% as the industrial floor, so a supplier quoting a density figure without stating the class is quoting a number that cannot be compared.
The tungsten carbide grade page covers what the cobalt-to-grain-size axes mean commercially, and tungsten production covers the route from ore to the metal powder that this page starts with. The tungsten suppliers page covers the metal end of this chain, which is where the powder comes from.
Methodology
Figures are taken from the two sources below and from arithmetic performed on them, which is labelled where it appears. The 6.13% theoretical carbon content of tungsten carbide was computed from atomic masses (183.84 and 12.011) rather than quoted. The 5.517% total carbon in a 90 wt.% tungsten carbide grade is from the Stanciu review’s EDS table and is not our own measurement; using it to check the stoichiometric figure is our arithmetic.
The Stanciu review is a laboratory study of reactive sintering, so its density and grain-size numbers describe experimental samples, not production parts. Where a fact comes from work that review cites rather than from the review itself — the Trung graphite addition — this is stated in the sentence.
Sources
- Stanciu, V.I., Mégret, A., Mouftiez, A., Vitry, V., Delaunois, F., “Reactive Sintering of Cemented Carbides,” Alloys 4(3), 15 (2025) — carburising temperature, agglomeration, milling oxygen, eta-phase mechanism, grain growth inhibitor, 1,762/1,809 HV30, 10.9 MPa·m^1/2, 90%/70%/+99% density, reactive sintering cycle. https://www.mdpi.com/2674-063x/4/3/15
- Cahill, J.T. et al., “Suppressing eta-phase development in steel-cemented tungsten carbide,” OSTI (2018) — eta phase as carbon-deficient MxWyC with x+y=6; the Trung graphite addition and its 94.5% density ceiling. https://www.osti.gov/servlets/purl/1488769
- U.S. Geological Survey, Mineral Commodity Summaries 2026: Tungsten, February 2026 — 60% of consumption in cemented carbide, China 67,000 t and 2.5 Mt reserves, import sources, Rotterdam price series, February 2025 export controls. https://pubs.usgs.gov/periodicals/mcs2026/mcs2026-tungsten.pdf
Related
- SpecificationTungsten Carbide: A Grade Is Two NumbersTungsten carbide is a powder, a compound and a cemented composite. A grade is cobalt against grain size, and one ISO code can carry different numbers.
- UsesTungsten Carbide Uses: Why the Hardest LosesDiamond, cubic boron nitride and ceramics all beat tungsten carbide on hardness, and each fails on a specific workpiece. The 80% share is chemistry.
- SuppliersTungsten Carbide Manufacturers: Three VerticalsThe largest carbide makers do not buy powder: they make it from oxide or from ore they dug. Below them sits a pressing tier with no public roster.
- Tungsten · Critical MineralsTungsten Metal: Ten Kilograms, Not a TonneTungsten concentrate and APT are quoted per metric ton unit of oxide, ten kilograms, and the licence tests are cumulative rather than one threshold.