Tungsten Production: Where the Acid Goes
The routes differ in where acid enters the flowsheet. The art has pushed that point almost to zero; what remains is a liquor too dilute to boil cheaply.

On this page
Tungsten production has more than one process route in the literature, and they are usually described as competing chemistries. The more useful way to read them is by where acid enters the flowsheet, because that single position sets the reagent bill, the waste stream and the equipment.
The classical route puts acid in the middle, to make solvent extraction work. The newer routes push it to the front or remove it. The direction of travel is consistent; the accounts are not yet closed.
| Route | Where acid goes | Status in the review |
|---|---|---|
| Classical | Added before solvent extraction, to reach pH 2 to 3 | State of the art |
| Acidic leaching | In the leach itself, as nitric and phosphoric acid | Studied, not yet standard |
| Direct alkaline extraction | Nowhere | Pilot and industrial tests run |
| Biosorption | Added to about pH 1, for adsorption onto a biosorbent | Studied, on scrap |
The classical tungsten production route pays for the acid twice
Leaching comes first, and it is done in alkali. The review describes the step as usually performed with a large excess of NaOH or NaCO3 at an elevated temperature and high pressure in steel autoclaves
, and adds a cost that is easy to overlook: the treatment in autoclaves consumes large amounts of energy
. Reagent and energy are both spent before any purification begins.
| Step | Reagent or condition | What leaves the plant |
|---|---|---|
| Leaching | Excess NaOH or Na2CO3, autoclave | Residue |
| Purification | Precipitation | Sludge carrying tungsten |
| Extraction | Acid to pH 2 to 3, then solvent or resin | Spent salts |
| Crystallisation | Evaporation | Water vapour and the energy |
Purification is by precipitation, not by extraction. The sodium tungstate solution is purified by precipitation in order to remove the main impurities like Si, Mo, As, Sb, Bi, Pb and Co
, and the review’s concern at this stage is tungsten lost into the sludge.
Extraction comes after that, and it is where the acid enters. Most industrial extractants work best at pH 2 to 3, and the leachate is strongly alkaline, so the liquor is acidified first. The consequence is stated flatly: lots of acid is needed to neutralize and acidify the leach liquor and the valuable alkali (Na2CO3 or NaOH) and acid (H2SO4 or HCl) become useless inorganic salts
. The alkali that dissolved the tungsten and the acid that neutralised it both leave as salt.
Ion exchange is the alternative at this point, using strongly alkaline resins that adsorb the tungstate without acidification, which the review raises as a question of which feed suits which method rather than as a settled preference. The review frames the choice between the two as an open question rather than a settled one.
Acid at the front of the flowsheet
Scheelite can also be leached in acid directly. The review records that the ore can be treated in an acidic leaching step with hydrochloric acid to produce tungstic acid
, and that this approach has a specific failure: a colloidal layer of tungstic acid coats the unreacted particles and hinders the reaction.
The workaround that gets mentioned with it is a mixture of nitric and phosphoric acid. The phosphoric acid acts as a chelating agent and avoids tungstic acid precipitation, and the result is a phosphotungstic acid solution that goes to solvent extraction as it is. Because the leachate is already acidic, there is no further acid needed prior the solvent extraction step
, and the raffinate returns to the leach.
The economics move in the right direction: acid consumption and wastewater volume both fall sharply. The status does not. The review places this route among concepts that are not (yet) state-of-the-art
, which is the distinction that matters if the question is what a refinery actually runs today.
The route that removes the acid entirely
The third route starts from the observation that the acid step is not only expensive but incomplete. In acidic solvent extraction, anionic impurities of phosphorus, arsenic, silicon and tin cannot be removed, because of the formation of heteropoly acid
, and precipitating them takes tungsten with them.
Extracting directly from the alkaline liquor avoids both problems. The original attempts were held back by poor phase separation and by the dilution of the product stream: a relatively low tungsten concentration in the strip liquor (aprox. 100 g/l) resulting in high energy consumption in the following crystallization of APT by evaporation
.
What changed is scale. The route was tested at pilot and industrial size, and the results were measured. A study cited in the review converted a quaternary ammonium chloride into a carbonate salt and ran multi-stage mixer-settler pilot tests and multi-stage annular centrifugal extractor industrial tests over an extended period. The pilot results the review tabulates are for caustic leach liquor from wolframite concentrate; it does not state the feed for the industrial tests. The reported results are worth stating in full:
- Extraction rate.
The extraction rate reaches 98 %.
- Impurities.
Other impurities like P, As, Si and Sn are almost removed quantitatively.
- Acid.
There is no consumption of acid
, and no precipitation step for phosphorus, arsenic and silicon is needed. - Recycle. The organic phase and the aqueous phase run as closed cycles, as do the sodium carbonate and sodium hydroxide.
- Cost.
the overall costs can be reduced by about US$ 400 per ton APT
.
Molybdenum is co-extracted and has to be removed in a following precipitation step, so the route is several stages shorter than the classical one, and not more than that.
The bottleneck that survives every tungsten production route
The classical route and the direct alkaline route both end at the same operation: crystallising ammonium paratungstate by evaporating water. The biosorption concept in the same chapter skips it, going from tungsten trioxide to tungsten carbide by reduction and calcination. That step has no chemistry to optimise, only a concentration to work with, and concentration is where the routes differ.
The classical route reaches crystallisation after solvent extraction. The direct alkaline route reaches it through an extractant that leaves tungsten more dilute, and the 100 g/l figure belongs to that route and that paper, not to the process in general. A weaker feed means more water to evaporate per tonne of salt, and that is the cost the acid saving is traded against.
In tungsten production the chemistry has been pushed close to its limit. What remains is a separation problem, and separation is priced in energy.
The loss that happens before any of this
Beneficiation sits in front of the flowsheet and carries the largest single figure in the review: considerable losses of about 10 – 40 % of the tungsten content of the ore
. The range is broad because it depends on the ore and the circuit, which is why it is worth asking for the number rather than assuming the favourable end.
That figure comes from the same review, and it explains why scrap is a feedstock in its own right. A spent tool has already been concentrated, leached, purified and crystallised once, so reprocessing it skips the stage where the 10 to 40% disappears. The USGS lists scrap alongside concentrate and the intermediate salt as material that American converters accept, and tungsten suppliers sets out which companies those are.
What the salt does not decide
Ammonium paratungstate is a crystallised salt with a defined composition, which is why it is the form that trade and licensing attach to. It fixes tungsten content and impurity profile, and nothing about the powder.
The American consumption figures show where that powder goes: the USGS estimates that about 60% of tungsten consumed in the United States was used in cemented carbide parts for cutting and wear-resistant applications, with the remainder used in alloys and specialty steels, and in electrodes, filaments and wires for electrical, heating, lighting and welding applications. Powder is made by reducing the salt or its oxide and then carburising, and those steps set particle size, particle size distribution and carbon content. Those are the numbers a carbide buyer specifies. Tungsten carbide sets out how a grade is written down, and tungsten covers the element, its price series and the export controls that name the salt.
What to ask before specifying a tungsten route
- Where the acid enters. Classical, acidic leaching or direct alkaline extraction — the answer determines the reagent bill and the waste stream.
- Whether the route is running or published. Two of the three are described in the literature as not yet standard, and a supplier’s route may not be the one in the review.
- The tungsten concentration entering crystallisation. This sets the evaporation energy, and it differs by route.
- The beneficiation loss, as a percentage. It is the largest figure in the chain and it is fixed before any chemistry happens.
- Whether the purchase is the salt or the powder. One has a composition, the other a particle size distribution, and they arrive as different documents.
Methodology
The process description, the reagent and energy costs of autoclaving, the precipitation step and its impurity list, the acidification and its salt waste, the ion-exchange alternative, the acidic leaching route and its colloidal-layer problem, the heteropoly-acid limitation, the direct alkaline extraction results including 98%, quantitative impurity removal, the closed cycles and US$ 400 per ton, the 100 g/l figure and the 10 to 40% beneficiation loss all come from the MSP-REFRAM review cited below, which is a review of published practice rather than any single plant’s flowsheet.
The USGS summary is used only for the statement that American converters accept scrap, concentrate and the salt as feed. The 100 g/l figure is attributed to the direct alkaline route and to the paper that reported it, not to crystallisation in general; the review gives no corresponding figure for the classical route, and this page does not invent one.
Sources
- MSP-REFRAM, Innovation potential in the recovery of refractory metals from primary sources, D2.3, hydrometallurgy of tungsten, pp. 22–26 (leaching conditions, autoclave energy, precipitation purification, acidification losses, ion exchange, acidic leaching, heteropoly acids, direct alkaline extraction, 100 g/l, US$ 400 per ton, beneficiation losses). https://prometia.eu/wp-content/uploads/2020/12/MSP-REFRAM-D2.3-Innovation-potential-recovery-refractory-metals-primary-sources.pdf
- U.S. Geological Survey, Mineral Commodity Summaries 2026: Tungsten, February 2026 (converters and the forms they accept as feed). https://pubs.usgs.gov/periodicals/mcs2026/mcs2026-tungsten.pdf
Related
- SpecificationTungsten Metal: Ten Kilograms, Not a TonneTungsten concentrate and APT are quoted per metric ton unit of oxide, ten kilograms, and the licence tests are cumulative rather than one threshold.
- UsesTungsten Uses: 60% of US Demand, One ProductIn the US, 60% of tungsten demand goes to cemented carbide. The other 40% splits into alloys and specialty steels, electrodes and wires, and chemicals.
- SuppliersTungsten Suppliers: Countries, Not CompaniesTungsten supplier lists mix mine output, concentrate and APT. The only comparable ranking is the country table, and most producers publish no capacity.
- Metallurgy · Critical MineralsAntimony Production: The Grade Picks the FurnaceSix routes make antimony metal, and the concentrate grade decides which one runs. The route that dominates yields about 99.4%, not four nines.